I.
Intruduction
Shandong lunbo
luminous products co.,ltd has been leading the way of applying
the photoluminescent pigment to glaze to make photoluminescent
glaze which can be widely used in the production of ceramic
floor tiles,ceramic internal wall tiles and enamel signs
and give luminous products excellent indicating and beautifying
effect.
The photoluminescent
glaze is composed of basic glaze,photoluminescent pigment
as well as little additives and can be used directly to
produce luminous products after complete blend.It can be
applied to artistic tiles of internal wall,indication tiles,household
ceramics as well as glass utensils.
II.
Performance
Index
|
Index
Item
|
Firing temperature(℃)
|
Firing time (minute)
|
Luminance after
1 min
≥
|
Luminance after
60 min
≥
|
Afterglow time
(min) ≥
|
|
TGB
|
TGB-45H
|
1100—1180℃
|
≤40
|
680
|
16.0
|
2000
|
|
TGB-45M
|
1000—1080℃
|
≤40
|
680
|
16.0
|
2000
|
|
TGB-45L
|
900—1000℃
|
≤45
|
580
|
14.0
|
1800
|
|
TGG
|
TGG-45L
|
900—1000℃
|
≤45
|
900
|
11.0
|
1200
|
|
TCB
|
TCB-35
|
800—850℃
|
≤10
|
600
|
16.0
|
1500
|
Note:
The thickness of the photoluminescent glaze layer is suggested
0.2-0.4mm.
III.Usage
Luminous Enamel Glaze
Photoluminescent enamel glaze had better be doped on the
surface of the fired white enamel glaze layer to form the
luminescent patterns. The doping and firing technologies
of white enamel layer are like those of traditional white
enamel.
1. Mix the PL enamel glaze with water (the weight ratio
is 1:0.5-0.6) in the ball milling pot for 5 minutes to get
glaze slurry.
2. Dope glaze slurry on the surface of the fired white glaze
layer to get luminous layer, the thickness of this luminous
layer is 400-500μm.
3. Dry it.
4. Fired 2-4 minutes at 800-850℃, luminous enamel product
is got.
5.In order to obtain more smooth surface, a layer of thin
transparent glaze can be doped on the luminous glaze layer.
6. Luminous glaze can also be mixed with certain amount
of screen-printing ink to form luminous patterns through
screen-print technology.
SUGGESTIONS
1. Do not grind the PL pigment with metal material, otherwise
the luminous effect will be affected.
2. Add 1-2%(by weight) of baste to increase the fluidity
and suspension of glaze, if you find deposition during usage.
3. Using TCB-35 transparent enamel glaze manufactured by
our company, you can get better effect.
Luminous Ceramic Glaze
Adopt different technological steps according to different
luminous ceramic products.
Luminous internal wall glaze tile
1. Ball mill TGB-45M series PL ceramic glaze with water
(the weight ratio is 1:0.6-0.7) in ball milling machine
for 20 minutes to get the glaze slurry.
2. To form a layer of luminescent glaze 200-400μm by spraying,
spraying and pouring method.
3. Dry it.
4. Fired 35-50 minutes at 1000-1080℃, luminous internal
wall glaze tile is got.
Luminous
floor tile(pattern tile)
1. Mixing TGB-45H series luminous ceramic glaze with certain
amount of screen-printing oil can get the screen-printing
slurry.
2. Screen print luminous glaze slurry on the unfired floor
tile's white glaze, then get luminous pattern.
3. Pour a layer of transparent glaze on the surface of the
pattern.
4. Fired 35-45 minutes at 1100-1180℃, luminous design tile
product is got.
Luminous internal wall design tile (fired
for three times)
1. Mixing TGB-45L series luminous ceramic glaze with certain
amount of screen-printing oil can get the screen-printing
slurry.
2. Screen print luminous design on the surface of the fired
white internal wall glaze tile.
3. Pile transparent dry glaze powder on the luminous design
with screen.
4. Fired 40-50 minutes at 900-1000℃, internal wall tile
with protuberant design is got.
SUGGESTIONS
1. Do not grind the PL pigment with metal material, otherwise
the luminous effect will be affected.
2. If you
find deposition during using, add 2%(weight) of baste to
increase the fluidity of glaze.
3. You had better adopt suited transparent glaze produced
by our company when producing luminous tile.
|